Engineering tool

Welding procedure qualification planner

Describe the butt weld test you plan to make. The planner shows the thickness range and steels the approval will cover, the limits that apply in production, the tests and impact notch positions the test plate needs, and the values the results must reach, from the CCS Rules for welding procedure approval.

01

Test conditions

Joint type of the test
B, single-sided, without backing
Welding passes
Heat input class (kJ/cm)
02

Additional conditions (optional)

Welding positions tested
Approved thickness, butt and T joints12.5 – 50mm
The steel has a minimum yield strength of 355 N/mm² or more, so an approval on a butt weld does not carry over to fillet welds. A fillet weld test to the structural requirements is needed (3.1.4.13).
03

Approved range and production limits

Fillet welds are covered by the same range, applied to the thickness of both plates.
Joint types the approval covers: B, A, C, DTable 3.1.4.13
Welding positions: only the position tested3.1.4.8
For a butt weld between plates of unequal thickness, the range is applied to the thinner plate3.1.4.5 (4)
04

Steels the procedure covers

Hover over a grade to see why.
OrdinaryABDE
Grade 32AH32DH32EH32FH32
Grade 36AH36DH36EH36FH36
Grade 40AH40DH40EH40FH40

Covered Confirm with the society Not covered

05

Tests on the test plate (3.2.4.1)

Transverse tensile specimens: 2.
Transverse bend specimens: 4, two face and two root.From 12 mm thick, 4 side bend specimens may replace them.
Macro section: 1.
Hardness test: 1, taken with the macro section.
Longitudinal all-weld-metal tensile specimen: 1, only if the consumable is not yet approved.
Impact tests: sets of 3 specimens at these notch positions.
Impact notch positions
Surface sidea, b, c
Root sidea

a weld centre, b fusion line, c heat affected zone 2 mm from the fusion line, d 5 mm, e 10 mm. Position d is added only when the approval will be used for important offshore structure joints (note 2).

06

What the results must show (3.2.5)

Joint tensile strength not less than 490 N/mm², the minimum for the base metal.
After bending, no opening defect longer than 3 mm in any direction on the tension surface.
Impact test temperature: 0 °C.
Average impact energy not less than 47 J.Manual or semi-automatic flat, horizontal and overhead welds: 47 J. Vertical welds and automatic welding: 34 J allowed.
Hardness not above HV350.
Macro section: good weld profile, full penetration, no cracks or lack of fusion.
Visual and non-destructive examination to ISO 5817 class B, with excess weld metal, convexity and root sag accepted to class C.
Interpretations and production conditions (9)
  1. A multi-pass procedure cannot be used for single-pass welds (3.1.4.2).
  2. A procedure approved on normalised, as rolled or controlled rolled steel generally covers TMCP steel too, but not the other way round (3.1.4.3 (5)).
  3. Each condition above stands on its own. A change beyond the covered range in any one of them generally needs a new approval test (3.1.4.1).
  4. Preheat temperature not lower than in the test, and interpass temperature not higher than in the test (3.1.4.11).
  5. If the test used post weld heat treatment or ageing, production needs it too (3.1.4.12).
  6. A change of current type (direct, alternating, pulsed) or of polarity normally needs a new approval (3.1.4.10).
  7. Consumables: the same grade as in the test, suffix included. For processes above 50 kJ/cm the rule gives no coverage statement (3.1.4.7).
  8. Shielding gas: a change of composition or mixing ratio is allowed only within the groups of Table 2.5.1.3 or 2.9.2.4 (3.1.4.7).
  9. An approval made with workshop primer covers welding without primer, but not the other way round (3.1.4.14).
What this planner covers

CCS Rules for Materials and Welding 2021, Part 3 Chapter 3: the approved thickness range (Table 3.1.4.5a), the steels a test covers (3.1.4.3), the joint types, pipe diameter, heat input, throat thickness and welding positions the approval covers (3.1.4.5 to 3.1.4.14), the test specimens and impact notch positions (3.2.4.1), and the acceptance requirements (3.2.5): tensile, bend, impact temperature and energy, hardness and macro examination. It covers hull steels A, B, D, E and the AH, DH, EH and FH grades of 32, 36 and 40.

What it does not cover

Fillet weld procedure tests, welder qualification, aluminium and stainless steel, and test joints between two different steels (the rules take the impact specimens from the lower toughness side). The conditions in production are listed only and are not checked against your procedure. The tool does not replace the approval, which is witnessed by your surveyor.

Source

Every table cell and clause above was read from the page images of the CCS Rules for Materials and Welding 2021. This is the CCS rule, not an IACS unified requirement: IACS UR W28 needs a free IACS login to download and was not checked. Your society's own rules govern.

This planning aid does not constitute an approval. The approval certificate issued by your classification society states the approved range. For plate ready to ship, contact us. Request a quote

Common questions
Why do fillet welds need a multi-pass test?
Table 3.1.4.5a lists fillet welds only in the multi-pass column. A single-pass test gives a range for butt and T joints and does not list fillet welds.
Why does heat input change the result?
Above 50 kJ/cm the rules cover fewer steels, cap the approved thickness at the tested thickness, and add an impact notch position. Above 200 kJ/cm they add one more.
Why does the planner say to confirm some steels with the society?
For steels of lower strength, clause 3.1.4.3 (2) gives the strength range but says nothing about toughness. If the steel to be welded is a tougher grade than the test steel, the rule does not answer, so the planner does not either.